Test method

    EN 1849-2 - Flexible sheets for waterproofing - thickness and mass per unit area - plastic and rubber sheets

    Testing · NAC-037-TL

    In short

    EN 1849-2 - Flexible sheets for waterproofing - thickness and mass per unit area - plastic and rubber sheets. Amstelfy's laboratory determines thickness and mass per unit area of plastic and rubber sheets according to EN 1849-2 under its ISO/IEC 17025 accreditation (NAC-037-TL). The method is typically part of initial type testing, ETA test programmes or factory production control verification; results are reported in English for manufacturers across Europe.

    What EN 1849-2 determines

    EN 1849-2 determines the thickness and the mass per unit area of plastic and rubber waterproofing sheets. For these membranes thickness is the primary design and identification value, since the polymer film itself carries the function and the strength of homogeneous sheets is expressed as a stress over that thickness. The standard measures thickness with a gauge under defined contact pressure, and for sheets with an embossed, profiled or fleece-backed surface it distinguishes the overall thickness from the effective thickness of the waterproofing layer, which is the value that matters for watertightness, welding and durability. Mass per unit area is determined by weighing a piece of known area and, together with thickness, gives the density and reveals filler content or a backing fleece. Both are declared with tolerances and are checked in factory production control on every production run.

    Specimens, conditioning and procedure

    Specimens are cut from the sheet across its width, conditioned at the standard temperature, and measured with a thickness gauge whose foot diameter and pressure are fixed in the standard, at points distributed over the width away from edges and selvedges. Where the sheet has a textured surface, a lacquer or a laminated fleece, the effective thickness of the waterproofing layer is determined as the standard describes and reported separately from the overall thickness. For mass per unit area, specimens of accurately measured area are weighed and the mass is divided by the area. Means and the variation across the width are calculated and compared with the declared nominal values and tolerances.

    What the report states

    For each specimen the report lists the gauge readings and their mean in mm, the effective thickness where a texture or backing makes it relevant, and the mass per unit area in g/m², alongside the nominal values and tolerances the manufacturer declared and a conformity statement. Because these two numbers identify the compound and the production run, they head every later test report in the programme.

    Where the result is required

    Required by EN 13956, EN 13967, EN 13984 and EN 13859-1 and EN 13859-2 as declared characteristics and as the identification of plastic and rubber sheets under test, and used in factory production control on extrusion and calendering lines. Roofing and tanking specifications set minimum effective thicknesses for welded membranes, and the thickness is the divisor for the strength of homogeneous sheets in EN 12311-2 method B. Bitumen sheets are measured by EN 1849-1.

    What we assess

    • thickness and mass per unit area

    Products covered

    • plastic and rubber sheets

    Accreditation status

    ActivityStandardAccreditationValidityOn scope
    TestingISO/IEC 17025:2017NAC-037-TLvalid until 2 December 2028Yes
    Product certificationISO/IEC 17065:2012NAC-026-PPSvalid until 31 January 2030No
    Validation & verificationISO/IEC 17029:2019NAC-006-VVvalid until 31 January 2030No

    Route to market

    This test method is used inside initial type testing, ETA assessment programmes and factory production control verification. Amstelfy reports it as an accredited test under NAC-037-TL, either stand-alone or as part of a complete test programme.

    How it works

    1. 1

      Send the standard number, product description and intended use

    2. 2

      We confirm the applicable test series, sample quantities and timeline

    3. 3

      Samples are delivered to Veilmeesterweg 20, 1187 ZW Amstelveen (Mon-Fri 09:00-17:00)

    4. 4

      You receive the report in English, written for the TAB, Notified Body, evaluation service or programme operator.

    Frequently asked questions

    Yes - it is listed on the ISO/IEC 17025 testing scope NAC-037-TL.

    The thickness of the layer that actually keeps the water out, excluding surface texture, a decorative lacquer or a bonded fleece that does not contribute to watertightness. For a profiled or fleece-backed sheet it is smaller than the overall thickness measured with a gauge, and it is the value that specifications for welded membranes refer to. The standard describes how it is determined.

    Together they give the density of the sheet, which identifies the compound: a heavily filled PVC or a polyolefin with a different filler loading shows up as a change of mass at the same thickness. A backing fleece also adds mass without adding effective thickness. Factory production control uses both values to detect drift in the formulation or the line settings.

    Part 1 for bitumen sheets lets the surfacing decide whether thickness or mass per unit area is declared, because granules spoil a thickness reading. Part 2 for plastic and rubber sheets always declares thickness, adds the concept of effective thickness for textured or backed sheets and uses mass per unit area as an identification and density check. The gauge principle is the same.

    Related standards

    All Waterproofing membranes, roof underlays & liquid-applied systems testing