Test method

    EN 1928 – Membrane watertightness test

    Flexible sheets for waterproofing - watertightness

    Testing · NAC-037-TL

    In short

    EN 1928 - Flexible sheets for waterproofing - watertightness. Amstelfy's laboratory determines watertightness of bitumen, plastic and rubber sheets according to EN 1928 under its ISO/IEC 17025 accreditation (NAC-037-TL). The method is typically part of initial type testing, ETA test programmes or factory production control verification; results are reported in English for manufacturers across Europe.

    What EN 1928 determines

    EN 1928 determines the watertightness of flexible waterproofing sheets: whether water under a given pressure passes through the sheet within a given time. Method A is the low-pressure procedure used for roofing sheets and underlays: the specimen lies on a support with a coloured absorbent paper beneath, water is applied from above at a modest pressure and any passage of water shows as a stain on the paper. Method B is the high-pressure procedure for damp proof and tanking sheets: the specimen is clamped between flanges, loaded with water at the pressure the product standard specifies for the type, and the dry side is observed for water. In both cases the result is pass or fail at the pressure and time set by the product standard, and the test is repeated after ageing to show durability.

    Specimens, conditioning and procedure

    Circular specimens are cut from the sheet away from edges and conditioned; seams can be included in the specimen where the product standard asks for joint watertightness. In method A the specimen is placed over the indicator paper on the perforated support, the cell is filled, the specified pressure is applied for the specified period and the paper is then inspected for colour change. In method B the specimen is clamped in the pressure cell over a support that lets water through, pressure is raised to the specified value, typically held for 24 h, and the underside is checked at intervals and at the end for drops or damp patches. Specimens that leak at the clamping edge are repeated.

    What the report states

    The report states the method, the pressure in kPa, the duration and, for each specimen, whether water passed, giving a pass or fail for the set. For CE marking the manufacturer declares watertightness as pass at the pressure the product standard assigns, for example the Type A or Type T pressure of the damp proofing standards, and repeats the declaration for the aged and chemically exposed condition where required.

    Where the result is required

    The core test of every flexible sheet standard: EN 13707 and EN 13956 for roofing, EN 13967 and EN 13969 for damp proofing and tanking, EN 13970 and EN 13984 for vapour control layers, EN 14695 for bridge decks, and EN 13859-1 and EN 13859-2 for underlays, which adapt method A to a low water head. It is also the check after impact, static loading, ageing and chemical exposure tests, so most other methods in the series end with an EN 1928 determination.

    What we assess

    • watertightness

    Products covered

    • bitumen, plastic and rubber sheets

    Accreditation status

    ActivityStandardAccreditationValidityOn scope
    TestingISO/IEC 17025:2017NAC-037-TLvalid until 2 December 2028Yes
    Product certificationISO/IEC 17065:2012NAC-026-PPSvalid until 31 January 2030No
    Validation & verificationISO/IEC 17029:2019NAC-006-VVvalid until 31 January 2030No

    Route to market

    This test method is used inside initial type testing, ETA assessment programmes and factory production control verification. Amstelfy reports it as an accredited test under NAC-037-TL, either stand-alone or as part of a complete test programme.

    How it works

    1. 1

      Send the standard number, product description and intended use

    2. 2

      We confirm the applicable test series, sample quantities and timeline

    3. 3

      Samples are delivered to Veilmeesterweg 20, 1187 ZW Amstelveen (Mon-Fri 09:00-17:00)

    4. 4

      You receive the report in English, written for the TAB, Notified Body, evaluation service or programme operator.

    Frequently asked questions

    Yes - it is listed on the ISO/IEC 17025 testing scope NAC-037-TL.

    Method A, with its low pressure and absorbent indicator paper, is used for roofing sheets, underlays and other products that see rain and standing water but no hydrostatic head. Method B, with the specimen clamped in a pressure cell, is used for damp proof and tanking sheets that must resist ground water under pressure. The product standard names the method and the pressure.

    Yes. A specimen can be cut so that a lap joint runs across it, and the joint is then subjected to the same pressure. This is required for some products and is a useful complement to the peel and shear tests of joints, because a seam can carry load yet still leak through a capillary channel along the overlap.

    The same pass or fail at the same pressure, on specimens that have first been heat aged to EN 1296, exposed to UV, heat and water to EN 1297 or immersed in chemicals to EN 1847, as the product standard requires. Durability of watertightness is declared separately from the unaged result in the Declaration of Performance.

    Related standards

    All Waterproofing membranes, roof underlays & liquid-applied systems testing