European Assessment Document

    EAD 340352-00-0104 - Fibre reinforced polymer kits made of a carbon or glass fabric and an epoxy resin

    Testing · NAC-037-TLCertification · NAC-026-PPSETA route

    In short

    EAD 340352-00-0104 is the EOTA European Assessment Document for fibre reinforced polymer kits made of a carbon or glass fabric and an epoxy resin. Amstelfy Technical Solutions tests wet lay-up FRP fabric systems against this EAD in its ISO/IEC 17025-accredited laboratory in Amstelveen (NAC-037-TL): cured laminate tensile properties, bond to concrete (pull-off, shear), durability and glass transition temperature. The test reports follow the EAD clause structure so a Technical Assessment Body can use them directly for the European Technical Assessment; Amstelfy does not issue ETAs itself. Within its ISO/IEC 17065 scope (NAC-026-PPS) Amstelfy can also act as the product certification body for this product family.

    What the EAD assesses

    EAD 340352-00-0104 applies to kits in which a dry carbon or glass fabric is saturated with an epoxy resin on the structure and cured in place, forming the composite only at the moment of application. The assessment must therefore cover what the installer produces, not just the raw fabric: the fibre areal mass and architecture, the cured laminate made under controlled conditions, the resin's glass transition temperature, and the bond of the cured layer to concrete or masonry. Properties are usually referenced to the dry fibre thickness so that the designer is not dependent on the resin fraction achieved on site. Confinement of columns, shear strengthening of beams and flexural strengthening of slabs are the uses covered, and the ETA gives the values required by the design guidelines for each.

    Assessment programme

    Fabric is characterised for mass per unit area, fibre type and weave, and the roving tensile properties. Laminate panels are laid up in the laboratory with the kit resin following the manufacturer's procedure; coupons cut from them are tested in tension in the principal fibre directions, bidirectional fabrics being tested according to EN ISO 527-4 and unidirectional ones with the method for unidirectional composites. Glass transition temperature is measured on cured resin. Bond is tested by pull-off from concrete and by single-lap shear of a bonded strip pulled from a concrete block. Durability series expose cured laminate and bonded specimens to heat, humidity, alkaline and saline solutions and freeze-thaw before retesting.

    What the report states

    Reported per fabric type: areal mass, laminate tensile strength and modulus both on the measured laminate thickness and on the equivalent dry fibre thickness, ultimate strain, glass transition temperature, pull-off strength with failure plane, and shear-bond force with the effective bond length observed. Durability results are retained-property ratios per condition. Characteristic values are derived from the scatter of each series, and the number of specimens behind every value is stated.

    Where the result is required

    Wet lay-up systems are chosen where geometry is irregular or curved: column wrapping for ductility and axial capacity, U-wraps for shear, strengthening around openings, and masonry walls and vaults, usually in combination with fibre anchor spikes assessed under EAD 331668. The ETA values feed CNR-DT 200, fib Bulletin 90 and national design annexes, and are the European counterpart of the data an ICC-ES AC125 programme provides for the same products in the United States.

    What we assess

    • cured laminate tensile properties
    • bond to concrete (pull-off, shear)
    • durability
    • glass transition temperature

    Products covered

    • wet lay-up FRP fabric systems

    Accreditation status

    ActivityStandardAccreditationValidityOn scope
    TestingISO/IEC 17025:2017NAC-037-TLvalid until 2 December 2028Yes
    Product certificationISO/IEC 17065:2012NAC-026-PPSvalid until 31 January 2030Yes
    Validation & verificationISO/IEC 17029:2019NAC-006-VVvalid until 31 January 2030No

    Route to market

    Products covered by an EAD are placed on the EU market with a European Technical Assessment issued by a Technical Assessment Body (TAB), followed by the AVCP tasks of a Notified Body and the manufacturer's Declaration of Performance and CE marking. Amstelfy performs the assessment tests, prepares the test reports in the EAD's clause structure and coordinates the test plan with the TAB; Amstelfy does not issue ETAs.

    How it works

    1. 1

      Send the standard number, product description and intended use

    2. 2

      We confirm the applicable test series, sample quantities and timeline

    3. 3

      Samples are delivered to Veilmeesterweg 20, 1187 ZW Amstelveen (Mon-Fri 09:00-17:00)

    4. 4

      You receive the report in English, written for the TAB, Notified Body, evaluation service or programme operator.

    Frequently asked questions

    No. ETAs are issued by Technical Assessment Bodies designated under the CPR. Amstelfy carries out the assessment tests in its accredited laboratory, prepares the test reports to the EAD's clause structure and coordinates the test plan with the TAB of your choice.

    The laboratory lays them up under controlled temperature and humidity using the kit resin and the manufacturer's written procedure, so that the test reflects the documented installation method. Panels made by the manufacturer can be accepted for comparison when their preparation is witnessed or recorded, but the ETA series are based on panels produced under laboratory supervision.

    The thickness of a site-made laminate varies with the resin quantity and roller pressure, while the fibre content per square metre is a controlled property of the fabric. Expressing strength and modulus on the nominal fibre thickness gives the designer values that do not depend on how thick the resin layer turned out.

    Yes, where the manufacturer claims it. Bond tests are then repeated on the masonry types to be declared, such as clay brick, tuff or stone with the specified mortar, because pull-off and shear failure in masonry occur in the unit surface rather than in the adhesive. Each substrate appears as a separate line in the ETA.

    Related standards

    All FRP, FRCM/CRM strengthening & FRP reinforcement testing