Test method

    EN ISO 527-3 - Plastics - tensile properties - films and sheets

    Testing · NAC-037-TL

    In short

    EN ISO 527-3 - Plastics - tensile properties - films and sheets. Amstelfy's laboratory determines tensile strength and elongation of films and sheets according to EN ISO 527-3 under its ISO/IEC 17025 accreditation (NAC-037-TL). The method is typically part of initial type testing, ETA test programmes or factory production control verification; results are reported in English for manufacturers across Europe.

    What EN ISO 527-3 determines

    EN ISO 527-3 is the specimen part of the tensile series for films and sheets less than 1 mm thick, whether extruded, cast or calendered. Thin materials cannot be cut into the dumbbells used for moulding compounds without edge damage, so the standard provides strip specimens with parallel edges and, for some materials, dumbbell shapes punched with sharp dies. Under the general principles of EN ISO 527-1, the strip is extended at constant speed and the tensile strength, stress and strain at yield, strain at break and, where required, the modulus are determined. Because films are oriented during manufacture, properties are determined in the machine and transverse directions, and the ratio between them is itself a quality indicator for extrusion and stretching processes.

    Specimens, conditioning and procedure

    Strips are cut from the film with a sharp blade or twin-blade cutter so that both edges are smooth and parallel; nicks cause premature tearing and low elongation. Thickness is measured with a precision gauge suited to films because the result is calculated on the cross-section. Specimens are conditioned in the standard atmosphere and tested in pneumatic or line-contact grips, often with rubber faces, to prevent slipping and grip breaks. At least five specimens per direction are tested at the speed selected from the EN ISO 527-1 series, typically a high speed for elongation of ductile films and a low speed when modulus is required with a non-contact or clip-on extensometer.

    What the report states

    Reported per direction: tensile strength in MPa and, where useful for thin films, force per unit width in N/mm; stress and strain at yield; strain at break in %; tensile modulus when measured; the thickness used in the calculation; and the number of specimens, with grip breaks excluded. The machine-to-transverse ratio shows orientation, and the curves are attached.

    Where the result is required

    The method serves packaging and agricultural films, vapour control layers, protective and construction films, and the plastic sheets used as liners and separation layers. Waterproofing sheets have their own tensile method in EN 12311-2 and geomembranes use wide-width testing, but material qualification, incoming inspection and ageing studies on films return to EN ISO 527-3 because it is sensitive to extrusion quality, orientation and plasticiser loss after UV or heat exposure.

    What we assess

    • tensile strength and elongation

    Products covered

    • films and sheets

    Accreditation status

    ActivityStandardAccreditationValidityOn scope
    TestingISO/IEC 17025:2017NAC-037-TLvalid until 2 December 2028Yes
    Product certificationISO/IEC 17065:2012NAC-026-PPSvalid until 31 January 2030No
    Validation & verificationISO/IEC 17029:2019NAC-006-VVvalid until 31 January 2030No

    Route to market

    This test method is used inside initial type testing, ETA assessment programmes and factory production control verification. Amstelfy reports it as an accredited test under NAC-037-TL, either stand-alone or as part of a complete test programme.

    How it works

    1. 1

      Send the standard number, product description and intended use

    2. 2

      We confirm the applicable test series, sample quantities and timeline

    3. 3

      Samples are delivered to Veilmeesterweg 20, 1187 ZW Amstelveen (Mon-Fri 09:00-17:00)

    4. 4

      You receive the report in English, written for the TAB, Notified Body, evaluation service or programme operator.

    Frequently asked questions

    Yes - it is listed on the ISO/IEC 17025 testing scope NAC-037-TL.

    The standard defines strip widths within a range and a minimum length so that the grip distance and gauge length can be set; a wider strip is used for highly oriented or embossed films to average local variations. The report states the width and the grip distance used because elongation values depend on them.

    Elongation at break is controlled by the weakest point along the edges, so a single nick, gel or thickness drop terminates the test early. Cutting quality and grip alignment matter more than for thick plastics. The standard requires the failure location to be recorded, and grip breaks are excluded from the statistics.

    Multilayer films that behave as one material can be tested as a whole, with the total thickness used for stress. Textile-reinforced or heavily coated products are more usefully tested by methods that report force per width, since the layered cross-section no longer gives a meaningful stress.

    Related standards

    All Plastics, composites & metals - material test methods testing