Test method

    EN ISO 10319 - Geosynthetics - wide-width tensile test

    Testing · NAC-037-TL

    In short

    EN ISO 10319 - Geosynthetics - wide-width tensile test. Amstelfy's laboratory determines wide-width tensile strength and elongation of geotextiles, geogrids and geocomposites according to EN ISO 10319 under its ISO/IEC 17025 accreditation (NAC-037-TL). The method is typically part of initial type testing, ETA test programmes or factory production control verification; results are reported in English for manufacturers across Europe.

    What EN ISO 10319 determines

    EN ISO 10319 is the reference tensile test for geosynthetics. A strip 200 mm wide, with a nominal gauge length of 100 mm between the clamps, is extended at a constant rate of strain of 20 % per minute until it breaks, and force and elongation are recorded throughout. The width is deliberately large: a narrow strip of a woven or a needle-punched nonwoven necks in and sheds load through its edges, whereas a 200 mm specimen behaves more like the product in the ground, where soil restrains it laterally. The method gives the maximum tensile force per unit width, the strain at that force and, on request, the force at specified strains that reinforcement design uses. Results are given for both directions, since most products are anisotropic. Geogrids are tested as whole ribs, normalised per metre width.

    Specimens, conditioning and procedure

    At least five specimens per direction are cut to EN ISO 9862 and conditioned where required; wet testing after soaking is an option for moisture-sensitive products. Each specimen is mounted in clamps wide enough to grip the full 200 mm without slippage or clamp breaks; roller, wedge or capstan jaws are chosen to suit the product. Strain is measured over gauge marks on the specimen with a contact or optical extensometer rather than from crosshead travel. The crosshead moves at 20 % strain per minute of the gauge length until rupture, the force-strain curve is recorded and the failure location is noted. Geogrid specimens contain a defined number of ribs, and the rib count per metre converts force to kN/m.

    What the report states

    The report gives, per direction, the tensile strength in kN/m (maximum force per unit width), the elongation at maximum force in percent and, where requested, the force at 2 % and 5 % strain or the secant stiffness, each with individual values, mean and coefficient of variation. Failure modes and any clamp breaks are stated. The manufacturer declares the mean with a tolerance at the 95 % confidence level in the Declaration of Performance.

    Where the result is required

    Tensile strength and elongation to EN ISO 10319 are required characteristics in every harmonised geotextile standard, EN 13249 to EN 13257 and EN 13265, whatever the function, and the method is the basis for the retained-strength ratios in the durability screening tests EN 12224, EN 12225, EN 12447, EN ISO 13438 and EN 14030. Seam strength under EN ISO 10321 is compared with it. For geogrid reinforcement the short-term strength from this test is the starting point from which creep, installation damage and durability reduction factors give the design strength.

    What we assess

    • wide-width tensile strength and elongation

    Products covered

    • geotextiles
    • geogrids
    • geocomposites

    Accreditation status

    ActivityStandardAccreditationValidityOn scope
    TestingISO/IEC 17025:2017NAC-037-TLvalid until 2 December 2028Yes
    Product certificationISO/IEC 17065:2012NAC-026-PPSvalid until 31 January 2030No
    Validation & verificationISO/IEC 17029:2019NAC-006-VVvalid until 31 January 2030No

    Route to market

    This test method is used inside initial type testing, ETA assessment programmes and factory production control verification. Amstelfy reports it as an accredited test under NAC-037-TL, either stand-alone or as part of a complete test programme.

    How it works

    1. 1

      Send the standard number, product description and intended use

    2. 2

      We confirm the applicable test series, sample quantities and timeline

    3. 3

      Samples are delivered to Veilmeesterweg 20, 1187 ZW Amstelveen (Mon-Fri 09:00-17:00)

    4. 4

      You receive the report in English, written for the TAB, Notified Body, evaluation service or programme operator.

    Frequently asked questions

    Yes - it is listed on the ISO/IEC 17025 testing scope NAC-037-TL.

    A 50 mm strip of a woven or needle-punched geotextile contracts sideways under load and the edge yarns or fibres carry less than their share, so the measured strength is lower and more variable than the product achieves when soil restrains it. The 200 mm width reduces that effect and gives a value closer to in-service behaviour.

    A minimum of five specimens in each direction, so ten strips of at least 200 mm width plus clamping length, taken from different positions across the roll. Products with high scatter, or programmes that also need wet tests or force at specified strains, require more. The cutting plan is agreed before sampling.

    It separates stiff reinforcement products, which mobilise their strength at a few percent strain, from extensible nonwovens that may stretch by half their length before failing. For separation and filtration the high elongation is useful survivability; for reinforcement the force at 2 % or 5 % strain is usually more relevant than the strength at break.

    Related standards

    All Geotextiles & geosynthetics testing