Test method

    EN 12224 - Geotextiles - resistance to weathering

    Testing · NAC-037-TL

    In short

    EN 12224 - Geotextiles - resistance to weathering. Amstelfy's laboratory determines weathering resistance of geotextiles, geogrids and geocomposites according to EN 12224 under its ISO/IEC 17025 accreditation (NAC-037-TL). The method is typically part of initial type testing, ETA test programmes or factory production control verification; results are reported in English for manufacturers across Europe.

    What EN 12224 determines

    EN 12224 is the screening test for the resistance of geotextiles to sunlight and rain in the period between installation and covering. Specimens are exposed in an artificial weathering apparatus with a xenon-arc source, which reproduces the solar spectrum, under a cycle of irradiation and water spray, until a radiant exposure of 50 MJ/m² has been accumulated, a dose taken to represent about one month of European summer exposure. The exposed specimens and unexposed reference specimens are then tensile tested and the retained strength is calculated as a percentage. The product standards use the result to assign a maximum period during which the product may be left uncovered on site. Polymers without UV stabilisation, thin products and some colours lose strength rapidly; the test ranks products on this basis without claiming to predict service life for permanently exposed applications.

    Specimens, conditioning and procedure

    Tensile specimens in the direction agreed, normally the machine direction, are cut to EN ISO 9862 with matching reference specimens from the same sample. The exposure specimens are mounted in the xenon-arc apparatus with the filter combination, irradiance, black-standard temperature, humidity and spray cycle set out in the standard, and are rotated or repositioned so that the dose is uniform. Exposure continues until the radiant exposure reaches 50 MJ/m² as measured by the apparatus radiometer. Exposed and reference specimens are then conditioned together and tested in tension by the method the standard prescribes, normally EN ISO 10319. Retained strength is the ratio of the mean exposed strength to the mean reference strength.

    What the report states

    The report states the retained tensile strength in percent, the mean strengths before and after exposure with their scatter, the radiant exposure reached and the apparatus settings. Under the geotextile product standards a retained strength of 80 % or more allows the product to remain uncovered for up to one month after installation; lower values reduce the permitted period to two weeks or, for products with poor or untested resistance, to one day. The manufacturer declares the resulting covering period.

    Where the result is required

    Resistance to weathering is part of the durability assessment in every harmonised geotextile standard, EN 13249 to EN 13257 and EN 13265, and in the geosynthetic barrier standards, where EN 12224 is cited for exposed membranes. It decides the covering period printed on data sheets and installation instructions, and it is called for by specifiers of erosion control mats, revetment filters and geotextiles that stay exposed between construction stages. Permanently exposed products need longer exposure programmes agreed separately.

    What we assess

    • weathering resistance

    Products covered

    • geotextiles
    • geogrids
    • geocomposites

    Accreditation status

    ActivityStandardAccreditationValidityOn scope
    TestingISO/IEC 17025:2017NAC-037-TLvalid until 2 December 2028Yes
    Product certificationISO/IEC 17065:2012NAC-026-PPSvalid until 31 January 2030No
    Validation & verificationISO/IEC 17029:2019NAC-006-VVvalid until 31 January 2030No

    Route to market

    This test method is used inside initial type testing, ETA assessment programmes and factory production control verification. Amstelfy reports it as an accredited test under NAC-037-TL, either stand-alone or as part of a complete test programme.

    How it works

    1. 1

      Send the standard number, product description and intended use

    2. 2

      We confirm the applicable test series, sample quantities and timeline

    3. 3

      Samples are delivered to Veilmeesterweg 20, 1187 ZW Amstelveen (Mon-Fri 09:00-17:00)

    4. 4

      You receive the report in English, written for the TAB, Notified Body, evaluation service or programme operator.

    Frequently asked questions

    Yes - it is listed on the ISO/IEC 17025 testing scope NAC-037-TL.

    No. The 50 MJ/m² dose represents roughly one month of summer sunlight, and the highest category under the product standards is permission to leave the product uncovered for one month. Products intended for permanent exposure, such as some erosion control mats, need extended exposure testing and a manufacturer's own durability statement.

    The xenon-arc with filters reproduces the full solar spectrum including visible light and near infrared, which affects specimen temperature and the behaviour of pigments and stabilisers. Fluorescent UV devices emphasise the short-wave band and are used in other standards; EN 12224 fixes the xenon-arc source so that results from different laboratories are comparable.

    Usually the machine direction, with a set of specimens for exposure and an equal set kept as unexposed references from the same roll. Both sets are tensile tested under identical conditions after exposure. Testing both directions is possible when the weaker direction governs the application; the cutting plan is agreed with the client.

    Related standards

    All Geotextiles & geosynthetics testing