    EN 1107-2 - Flexible sheets for waterproofing - dimensional stability - plastic and rubber sheets. Amstelfy's laboratory determines dimensional stability of plastic and rubber sheets according to EN 1107-2 under its ISO/IEC 17025 accreditation (NAC-037-TL). The method is typically part of initial type testing, ETA test programmes or factory production control verification; results are reported in English for manufacturers across Europe.

    What EN 1107-2 determines

    EN 1107-2 determines the dimensional stability of plastic and rubber waterproofing sheets, the PVC, TPO, EPDM, ECB and PIB membranes used on flat roofs and in tanking. Thermoplastic sheets are calendered or extruded under tension and frozen in that state; when a roof warms up the polymer relaxes and the sheet shrinks, mostly in the machine direction, which loads welded seams and pulls at upstands. Unreinforced sheets move most, fabric-reinforced sheets least. The method heats marked specimens freely in an oven for the period and temperature the standard fixes for these materials, then measures the change of the marked lengths after cooling. The result, in per cent per direction, is a direct indicator of how much a loose-laid or mechanically fixed membrane will pull on its fixings and seams over its first summers.

    Specimens, conditioning and procedure

    Specimens are taken from the roll at a distance from the edges and marked in both the longitudinal and transverse direction with reference points at a defined gauge length, measured at room temperature. Each specimen is laid flat on a talc-dusted plate so that it can move without restraint, placed in a ventilated oven at the test temperature, and kept there for the exposure period specified for plastic and rubber sheets, which is shorter than the 24 h used for bitumen sheets in Part 1. After the specimens have cooled to room temperature the distances between the marks are measured again. Curling, warping or bubbles are recorded, and the mean change in each direction is calculated.

    What the report states

    The report gives the mean linear change in per cent for the longitudinal and the transverse direction, with the sign indicating shrinkage or growth, the oven temperature and the exposure time, and any observation of warping. The value is declared in the Declaration of Performance where the product standard, for example EN 13956, requires it, usually against a maximum permitted change.

    Where the result is required

    Required by EN 13956 for plastic and rubber roofing sheets and cited by EN 13859-1 and EN 13859-2 for plastic underlays; also used for geomembranes and tanking sheets where a client wants to compare materials. Roofing system designers read the value together with the seam strength from EN 12317-2 to judge whether a membrane can be loose-laid under ballast or must be fully bonded. Bitumen sheets use Part 1 of the standard.

    What we assess

    • dimensional stability

    Products covered

    • plastic and rubber sheets

    Accreditation status

    ActivityStandardAccreditationValidityOn scope
    TestingISO/IEC 17025:2017NAC-037-TLvalid until 2 December 2028Yes
    Product certificationISO/IEC 17065:2012NAC-026-PPSvalid until 31 January 2030No
    Validation & verificationISO/IEC 17029:2019NAC-006-VVvalid until 31 January 2030No

    Route to market

    This test method is used inside initial type testing, ETA assessment programmes and factory production control verification. Amstelfy reports it as an accredited test under NAC-037-TL, either stand-alone or as part of a complete test programme.

    How it works

    1. 1

      Send the standard number, product description and intended use

    2. 2

      We confirm the applicable test series, sample quantities and timeline

    3. 3

      Samples are delivered to Veilmeesterweg 20, 1187 ZW Amstelveen (Mon-Fri 09:00-17:00)

    4. 4

      You receive the report in English, written for the TAB, Notified Body, evaluation service or programme operator.

    Frequently asked questions

    Yes - it is listed on the ISO/IEC 17025 testing scope NAC-037-TL.

    Calendering stretches the film and plasticised PVC keeps that strain until heated; losing plasticiser over time increases the effect. A glass fleece or polyester scrim locks the dimension, which is why reinforced sheets show small values. The test identifies the type of sheet and helps set installation rules for laps and perimeter fixings.

    No. Part 2 uses a shorter oven exposure because thermoplastic films relax fast and longer heating would add thermal degradation to the dimensional effect. Part 1 stores bitumen sheets for 24 h because the coating on a carrier relaxes slowly. Results from the two parts are therefore not compared with each other.

    Specimens that stick to the plate, curl up so the marks cannot be read, or are measured before cooling. Marks placed too close to the cut edge also distort the result because edges relax differently. Talc on the plate, careful cooling and gauge lengths placed centrally are the routine precautions, and anomalies are noted in the report.