Test method

    ISO 812 - Rubber, vulcanized or thermoplastic - low-temperature brittleness

    Testing · NAC-037-TL

    In short

    ISO 812 - Rubber, vulcanized or thermoplastic - low-temperature brittleness. Amstelfy's laboratory determines low-temperature brittleness of rubber compounds, elastomeric bearings and seals and waterstops according to ISO 812 under its ISO/IEC 17025 accreditation (NAC-037-TL). The method is typically part of initial type testing, ETA test programmes or factory production control verification; results are reported in English for manufacturers across Europe.

    What ISO 812 determines

    ISO 812 determines the temperature below which a rubber becomes brittle under sudden impact. Strip test pieces are clamped as cantilevers, cooled to the test temperature in a liquid or gaseous medium, and struck once by a striker moving at the specified speed; each piece is then examined for cracks, fractures or complete breaks. As temperature falls a rubber passes through its glass transition, and the impact test locates the point at which it can no longer deform fast enough to absorb the blow. The standard offers three procedures: A determines the brittleness temperature, the lowest temperature at which no test piece fails; B determines the temperature at which half of the pieces fail; C is a pass or fail test at a single specified temperature.

    Specimens, conditioning and procedure

    Test pieces are die-cut from sheet about 2 mm thick, or from the product where it is flat enough, in the shape and size the standard gives for the chosen type. A set is clamped in the holder of the apparatus and immersed in the cooled heat-transfer medium, normally a silicone fluid or alcohol bath, for the conditioning time before the striker is released. For procedures A and B the test is repeated at successive temperatures in steps until the failure boundary is bracketed; for procedure C only the specified temperature is used. After impact each piece is allowed to warm and is inspected with the naked eye for any crack visible on the surface.

    What the report states

    The report states the procedure used and, depending on it, the brittleness temperature in °C, the 50 per cent brittleness temperature derived from the failure counts at each step, or a pass or fail statement at the specified temperature with the number of pieces that failed. Test piece type, medium, conditioning time and striker speed are recorded. The value is a ranking index for cold flexibility, not a service limit.

    Where the result is required

    Low-temperature brittleness is specified for pipe and tunnel seals (EN 681-1 for cold-climate types), waterstops and expansion joint seals installed in northern and alpine regions, bearings under EN 1337-3 where low-temperature use is declared, roofing and gasket compounds, and many cable and automotive rubber parts. It supports cold-climate type designations in sealing product certification and complements the stiffness-based ISO 815-2 low-temperature compression set.

    What we assess

    • low-temperature brittleness

    Products covered

    • rubber compounds
    • elastomeric bearings and seals
    • waterstops

    Accreditation status

    ActivityStandardAccreditationValidityOn scope
    TestingISO/IEC 17025:2017NAC-037-TLvalid until 2 December 2028Yes
    Product certificationISO/IEC 17065:2012NAC-026-PPSvalid until 31 January 2030No
    Validation & verificationISO/IEC 17029:2019NAC-006-VVvalid until 31 January 2030No

    Route to market

    This test method is used inside initial type testing, ETA assessment programmes and factory production control verification. Amstelfy reports it as an accredited test under NAC-037-TL, either stand-alone or as part of a complete test programme.

    How it works

    1. 1

      Send the standard number, product description and intended use

    2. 2

      We confirm the applicable test series, sample quantities and timeline

    3. 3

      Samples are delivered to Veilmeesterweg 20, 1187 ZW Amstelveen (Mon-Fri 09:00-17:00)

    4. 4

      You receive the report in English, written for the TAB, Notified Body, evaluation service or programme operator.

    Frequently asked questions

    Yes - it is listed on the ISO/IEC 17025 testing scope NAC-037-TL.

    Procedure A finds the brittleness temperature by stepping the temperature down until a set of pieces all survive. Procedure B finds the temperature at which half the pieces fail, which needs more pieces and more steps but gives a statistically defined value. Procedure C only checks whether the material survives one specified temperature, which is what most product standards require.

    No. The impact test shows where the compound shatters under a sudden blow; a seal loaded slowly can function below that point, and a seal relying on recovery may fail above it. Specifications therefore pair ISO 812 with low-temperature compression set or stiffness tests. Treat the result as a comparative index for cold flexibility.

    Several strips are needed per temperature step, so procedures A and B consume more pieces than procedure C. Moulded sheet about 2 mm thick from one batch is the easiest source; flat regions of extruded profiles or waterstops can also be used. Pieces must be free of surface defects, which would otherwise initiate cracks.

    Related standards

    All Rubber, elastomers, sealants & adhesives testing