Test method

    ISO 2781 - Rubber, vulcanized or thermoplastic - density

    Testing · NAC-037-TL

    In short

    ISO 2781 - Rubber, vulcanized or thermoplastic - density. Amstelfy's laboratory determines density of rubber compounds, elastomeric bearings and seals and waterstops according to ISO 2781 under its ISO/IEC 17025 accreditation (NAC-037-TL). The method is typically part of initial type testing, ETA test programmes or factory production control verification; results are reported in English for manufacturers across Europe.

    What ISO 2781 determines

    ISO 2781 gives two methods for determining the density of solid rubber. Method A weighs a test piece in air and then immersed in water, using the Archimedes principle to obtain the volume; Method B uses a density bottle and is intended for small pieces or where Method A is unsuitable, for example when a test piece cannot be kept free of air bubbles. Density is a bulk property that depends on the polymer, the filler loading and the plasticiser content, so it is one of the quickest ways to confirm that a batch matches the compound that was type tested. It does not apply to cellular rubber, for which separate standards give apparent density.

    Specimens, conditioning and procedure

    A test piece of adequate mass with a smooth surface is cut from a sheet or from the product and cleaned; cut faces are acceptable, but a shape with as little surface area per unit mass as practicable is preferred because trapped air bubbles bias the immersion weighing. In Method A the piece is weighed in air on an analytical balance, then suspended in distilled or deionised water at a known temperature and weighed again, with any bubbles removed. In Method B the mass of the bottle filled with water, with and without the rubber pieces, is determined. Duplicate determinations are made and the water density at the test temperature is applied in the calculation.

    What the report states

    Density is reported in megagrams per cubic metre, which is numerically equal to grams per cubic centimetre, to three decimal places, with the method used, the test temperature and the liquid. The mean of two determinations is given with the individual values. Clients compare the result with the value in the compound specification or the type-test record, typically within a tolerance of a few hundredths.

    Where the result is required

    Density appears in compound specifications for bearings, seals, waterstops and expansion joint profiles and in the identification tests of ETA and certification programmes, where it is used alongside hardness and tensile properties to confirm that production rubber matches the assessed formulation. It is a routine factory production control test and is also needed to convert mass-based results, for example in ISO 1817 immersion tests, to volume change.

    What we assess

    • density

    Products covered

    • rubber compounds
    • elastomeric bearings and seals
    • waterstops

    Accreditation status

    ActivityStandardAccreditationValidityOn scope
    TestingISO/IEC 17025:2017NAC-037-TLvalid until 2 December 2028Yes
    Product certificationISO/IEC 17065:2012NAC-026-PPSvalid until 31 January 2030No
    Validation & verificationISO/IEC 17029:2019NAC-006-VVvalid until 31 January 2030No

    Route to market

    This test method is used inside initial type testing, ETA assessment programmes and factory production control verification. Amstelfy reports it as an accredited test under NAC-037-TL, either stand-alone or as part of a complete test programme.

    How it works

    1. 1

      Send the standard number, product description and intended use

    2. 2

      We confirm the applicable test series, sample quantities and timeline

    3. 3

      Samples are delivered to Veilmeesterweg 20, 1187 ZW Amstelveen (Mon-Fri 09:00-17:00)

    4. 4

      You receive the report in English, written for the TAB, Notified Body, evaluation service or programme operator.

    Frequently asked questions

    Yes - it is listed on the ISO/IEC 17025 testing scope NAC-037-TL.

    Method A, hydrostatic weighing, is the default for solid rubber pieces of adequate mass. Method B, the density bottle, is used for small pieces, cut strips or materials where air cannot be kept away from the surface during immersion. The two methods agree within the precision of the standard, and the report states which one was applied.

    A few grams of solid rubber are sufficient; a piece cut from a product or a sheet with a mass above the minimum stated in the standard works for Method A. For Method B several small pieces are used. Material with cells, voids or embedded fabric is not suitable and gives an apparent rather than true density.

    Because it is a quick way to detect formulation changes: a different filler loading or plasticiser content shifts the density measurably even when hardness is unchanged. Certification schemes and ETA programmes therefore list it among the identification characteristics checked during audits and in factory production control.

    Related standards

    All Rubber, elastomers, sealants & adhesives testing