Test method

    ISO 188 – Rubber heat ageing test

    Rubber, vulcanized or thermoplastic - accelerated ageing and heat resistance

    Testing · NAC-037-TL

    In short

    ISO 188 - Rubber, vulcanized or thermoplastic - accelerated ageing and heat resistance. Amstelfy's laboratory determines heat ageing of rubber compounds, elastomeric bearings and seals and waterstops according to ISO 188 under its ISO/IEC 17025 accreditation (NAC-037-TL). The method is typically part of initial type testing, ETA test programmes or factory production control verification; results are reported in English for manufacturers across Europe.

    What ISO 188 determines

    ISO 188 defines accelerated ageing and heat resistance tests for vulcanised and thermoplastic rubber. Test pieces are exposed, unstrained, to air at an elevated temperature for a set time and the resulting changes in hardness, tensile strength, elongation at break and other properties are measured against unaged pieces from the same sheet. Oxidative ageing and post-curing proceed faster at higher temperature, so the test compresses years of service into days; the standard warns that the ranking of compounds at a high ageing temperature may not match their ranking in service, so the chosen temperature should stay close to the service range. Two oven methods are defined, differing in air flow: Method A with a low air velocity and Method B with forced circulation at higher velocity.

    Specimens, conditioning and procedure

    Test pieces for the properties to be followed, usually ISO 37 dumb-bells and ISO 48 hardness pieces, are cut from the same sheet as the unaged reference set. They hang freely in a cell or cabinet oven, with the air change rate within the limits the standard sets, so that neither strain nor contact with other materials influences the result; different compounds are not aged together because volatile ingredients migrate. Temperature is selected from the preferred series in the standard, commonly 70, 100 or 125 °C, and duration from 24 hours to several weeks as the product standard requires. After exposure the pieces are conditioned in the standard atmosphere and tested in the same way as the references.

    What the report states

    The report gives the aged and unaged medians of each property and the change: hardness change in IRHD or Shore units, tensile strength and elongation at break change in per cent of the unaged value. Ageing temperature, duration, oven method and conditioning are stated. Product standards such as EN 681-1 and EN 1337-3 limit these changes, and the report records the result against the limit named by the client.

    Where the result is required

    Heat ageing to ISO 188 is required in EN 1337-3 for elastomeric bearings, in EN 681-1 for pipe seals, in specifications for waterstops, expansion joint seals, gaskets and profiles, and in the durability assessments of EADs covering bridge expansion joints and sealing components. Manufacturers also use it to compare antioxidant systems during compound development and as a periodic factory production control check on heat resistance.

    What we assess

    • heat ageing

    Products covered

    • rubber compounds
    • elastomeric bearings and seals
    • waterstops

    Accreditation status

    ActivityStandardAccreditationValidityOn scope
    TestingISO/IEC 17025:2017NAC-037-TLvalid until 2 December 2028Yes
    Product certificationISO/IEC 17065:2012NAC-026-PPSvalid until 31 January 2030No
    Validation & verificationISO/IEC 17029:2019NAC-006-VVvalid until 31 January 2030No

    Route to market

    This test method is used inside initial type testing, ETA assessment programmes and factory production control verification. Amstelfy reports it as an accredited test under NAC-037-TL, either stand-alone or as part of a complete test programme.

    How it works

    1. 1

      Send the standard number, product description and intended use

    2. 2

      We confirm the applicable test series, sample quantities and timeline

    3. 3

      Samples are delivered to Veilmeesterweg 20, 1187 ZW Amstelveen (Mon-Fri 09:00-17:00)

    4. 4

      You receive the report in English, written for the TAB, Notified Body, evaluation service or programme operator.

    Frequently asked questions

    Yes - it is listed on the ISO/IEC 17025 testing scope NAC-037-TL.

    Follow the product standard where one applies; otherwise choose a temperature from the preferred series that is above service temperature but below the point where the degradation mechanism changes, typically 70 °C for general elastomers and 100 °C or more for heat-resistant types. Durations of 72 or 168 hours are common for type testing, longer for durability studies.

    Volatile antioxidants, plasticisers and sulphur compounds migrate through the air from one compound to another and change the result in both directions. ISO 188 therefore requires separate cells or separate oven runs for different materials. Clients sending several compounds should expect them to be aged in parallel cells or in sequence.

    Yes. Pieces cut from the product are aged in the same way, and the properties are measured on test pieces cut from them afterwards, or the whole small component is aged and tested functionally. The report notes that test pieces came from a product, because cure gradients and inserts affect the change recorded.

    Related standards

    All Rubber, elastomers, sealants & adhesives testing